#General conclusion

In this thesis, the technological opportunities offered by SiC to fabricate thermal anemometers were investigated. The primary objective was to fabricate 3C–SiC-based MEMS heating devices, which required addressing three key challenges: their electrical insulation, suspension, and parallel wire placement. 3C–SiC thin films were grown heteroepitaxially on silicon and processed following different strategies: growth on an SoI wafer, burial of a highly resistive SiC layer beneath a more conductive one, and direct transfer of the SiC film onto glass. Of these, only the production of a SiC/Si/glass wafer stack made it possible to reliably produce suspended insulated SiC resistors. A DRIE etching process of the SiC/Si stack and a minimal isotropic etching step of the silicon underlayer proved to be the most direct way to electrically insulate the SiC resistors, while keeping freedom in their placement. This made it possible not only to measure the resistance of SiC wires, but also to use them as heaters for thermal anemometry. A static calibration was conducted in a turbulent boundary layer to obtain WSS values from the sensor response. The fabricated SiC/Si/glass sensor chips were tested in an onve, at 500 C° and 700 °C. While the SiC layer’s thermal properties allow for very high temperatures, the current implementation with borosilicate hinders the capability of the full system to perform in harsh environments.

#SiC as a sensing material for thermal anemometry

The specificities of using a semiconductor material like SiC for thermoresistive heaters were discussed. First and foremost, the key difference compared to metals is the non-monotonic resistance-temperature characteristic, implying a non-constant TCR. This decorrelates the wire’s total resistance from its average temperature, making the temperature profile for a given input current uncertain. The dopant concentration heavily influences the resistivity and TCR, the latter skyrocketing to more than 10 000 ppm/K when the dopant concentration is kept low. However, the benefits offered by these high levels of TCR are mitigated by large resistances, making the operation in a CTA and integration into acquisition instruments much harder. Currently, owing to the lack of suitable control electronics, the electrical resistance of the wires must be kept as low as possible. This can be achieved either by making the wires thicker and shorter, which reduces their efficiency as thermal probes,The thermal losses through conduction increase, undermining the flow-induced voltage fluctuation.

or by increasing the dopant concentration to lower the intrinsic resistivity, at the cost of a drastic reduction in TCR. Additionally, it was noticed that the non-constant TCR of the material requires the overheat point to be chosen carefully, to prevent the lateral measurement from cancelling out due to counteracting negative and positive TCR segments. However, SiC offers the advantage of handling much higher overheat points, making the probes themselves less prone to oxidation drifting, as well as reducing the risk of them accidentally melting due to improper handling.

A static calibration experiment in a turbulent boundary layer wind tunnel, using the SiC calorimeters operated by an in-house CTA controller, confirmed that SiC is usable as a thermal probe material to sense skin friction, and could potentially resolve turbulence’s frequency distribution, assuming further refinements in control electronics, while preliminary heating tests suggest that SiC does not degrade at 500 °C temperatures.

#Future engineering challenges

This work opens up various research opportunities for developing a technology platform for SiC thermal probes, by highlighting the remaining engineering bottlenecks that have yet to be overcome. First of all, climbing the TRL scale invariably implies substantial engineering efforts; this is particularly true for thermal SiC sensors, because of the double constraint: keeping SiC electric insulation while making the whole sensor chip harsh-environment compatible. The current bottleneck material of the fabricated sensor chips being the borosilicate glass, replacing it with fused silica would overcome the chip deformation past 550 °C. Packaging-wise, wire bonds protrude from the wall surface and are the main weakness of the sensor probes. Using through-substrate electric vias to route the contacts to the sensor chip’s backside would completely remove any wire-bonding protrusion as well as any metal on the surface, leaving a flush, metal-free sensing surface where only SiC is exposed to the flow. While this has been demonstrated by Mazzamurro et al. (2022)75 to route backside contacts with TSVs for metallic WSS sensors, achieving this for a SiC-based technology would significantly improve its integration capabilities in harsh environments.

Nevertheless, fully exploring the limits of SiC will require testing under considerably harsher conditions. Following the example of GRCs harsh environments test platform, in situ measurements under real operating conditions, or within real systems, will be key to raising the TRL. As the SiC technology presented in this work is still relatively new, a dedicated harsh environments infrastructure remains to be developed for its thorough evaluation. Combined with the packaging and chip design improvements as discussed above, such efforts open a genuine opportunity to harness the exceptional properties of silicon carbide for thermal anemometry.