#2.1 Resistors from 3C–SiC films epitaxially grown on silicon

#2.1.1 Heteroepitaxy of 3C–SiC on silicon wafers

Since the epitaxial SiC growths were conducted by Marc Portail’s team at CRHEA, the presentation of the reactor and growth conditions is adapted from the thesis work of Jiao (2012)76 and Arvinte (2016)122. All TEM characterizations were conducted at CRHEA as well.

#Growth conditions

All SiC thin films presented in this work were grown in the R1, an in-house CVD reactor based on the patented design of Leycuras (2000)6. It is a horizontal hot-wall reactor, where heating is applied by two independent graphite resistive elements,The independence of the resistances enables a thermal gradient in the reactor chamber.

placed above and below the deposition area, as shown in figure 2.1. Gases are inserted in a liner with a rectangular section area, to achieve laminar flow. The tilted wafer holder allows a laminar gas boundary layer to develop over the crystal surface, whose thickness is a key parameter controlling the growth rate. Here, the reactor was used in LPCVD mode, using a 200 mbar gas pressure. The deposition process is shown in figure 2.2. The SiC film growth, which occurs at 1 320 °C, is preceded by a carbonization step at a lower setpoint, around 1 100 °C, which creates nucleation sites on the silicon wafer surface. For the actual deposition step, the film growth rate only depends on the flow rate of silane (SiH4); for that specific reactor, it is typically 1.2 µm/h/sccm.

Water-cooled stainless steel chamber Upper graphite heating element Rotating substrate holder To vacuum pump Laminar flow Gas inlet Lower heating element Water-cooled stainless steel chamber Liner of rectangular cross-section
Figure 2.1.
Schematic of the CVD reactor used for the epitaxial growth of the SiC films, at CRHEA. Adapted from Jiao (2012)76, Mehregany et al. (1998)79.
2026-10-06T23:15:57.904002 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ Introduction o f   C H 3 8 Transition: C H   r a t e 3 8 diminution Introduction o f   S i H 4 Time → 20 1 100 1 320 Temperature (°C) Carbonization Precursors: H   +   C H 2 3 8 SiC growth Precursors: H   +   C H   +   S i H 2 3 8 4 H 2 H 2
Figure 2.2.
2-step growth of the 3C–SiC films. The time scale is arbitrary, as the growth step length depends on the desired thickness. The carbonization step usually lasts for 15 minutes. Adapted from Jiao (2012)76.

#Doping

Various levels of doping of the SiC layer were achieved in the reactor. For this work, all the samples were n-doped with various concentrations. To achieve it, an additional flow of N2 is introduced during the growth process. Nitrogen atoms substitute for carbon atoms, inserting an additional electron in the crystal lattice.

#Characterizations of the SiC films

The grown layers were cut, then TEM scanned, revealing the columnar growth of the SiC layer with numerous stacking faults (figure 2.3 (a)). The white dots visible in {figure 2.3 (b)} are artifacts introduced during thinning by the PIPS preparation process. The corresponding SAED pattern shown in figure 2.3 (c) presents localized dots indicating the monocrystalline structure of the grown epilayer.

Figure 2.3.
STEM - HAADF images of the SiC/Si interface.

(a) Low-magnification STEM–HAADF image of a 1.3 µm-thick SiC layer deposited on a silicon substrate.
(b) Higher-magnification STEM–HAADF image of the SiC/Si interface.
(c) Corresponding  pattern, confirming the textured nature of the layer.

#2.1.2 Development of a fabrication process for suspended 3C–SiC resistors

Because the AIMAN-FILMS group at IEMN had no prior research experience in processing silicon carbide, this work starts with the development of an etching recipe. The Oxford PlasmaLab 80 was chosen as the platform for this process, because of its availability and ease of use for a quick iterative roadmap. In order to converge towards an etching recipe that yields a good compromise between etch rate, wall slope and bottom surface quality, an iterative experimental process was defined. A masking pattern defining lines of various widths is created by metal evaporation and lift-off. The wafer is then manually cleaved to produce many test samples. A given RIE recipe is tested on one sample, which is cleaved again across the lines to be able to inspect a cross-section using a SEM. This makes it possible to measure the cavity depth, the selectivity of the etching rate of SiC relative to the metal mask, and the cavity slope. Iteratively, a new sample undergoes a variation of the recipe, and progress is tested the same way. The global process flowchart is shown in figure 2.4, while the results of each iteration are detailed in the following sections.

Si Al 3C–SiC 200 nm Evaporation of Al& lift-off Various RIE recipesfor SiC etching Test patterns etched 3C–SiC heteroetpitaxy on Si
Figure 2.4.
Line pattern masking and fabrication for RIE tests.

#Metal masking

Because O2 plasma forbids photoresist masking, a metal hard mask should be used instead. The literature suggests nickel and aluminum as the best metals for this case (Pan & Steckl 1990)123. Preliminary tests were executed to assess the selectivity and potential metal micro-masking. While aluminum produces alumina particles under O2 plasma that tend to settle on the bottom of the etch cavity (figure 2.5), nickel was found, in this particular case, to produce much more micro-masking, resulting in an unacceptable amount of grass in the etching cavity. The alumina beads produced by aluminum micro-masking were much more manageable.

The aluminum mask was patterned using an evaporation/lift-off process. First, a LOR 10A / AZ 1512 photoresist bilayer is spin-coated on the SiC/Si wafer, with respectively 4-minute 180 °C and 1-minute 110 °C bakes for each layer. The resist is exposed on a Kloé Dilase 650 UV laser writer, then developed in AZ 726 MIF solution. The result is a T-top profile suited for evaporation, as it lets the metal sit cleanly in the opening by preventing wall formation. After development, a bilayer of 20 nm chromium / 200 nm aluminum is evaporated on a Plassys MEB 550SL tool. The sacrificial chromium layer is used to chemically remove the mask in hydrochloric acid once the SiC layer is etched. The evaporated mask is finally lifted off in a heated SVC-14 bath.

Figure 2.5.
SEM details of the etching cavity, highlighting the micromasking effect with both aluminum and nickel masks.

(a) Etch cavity with aluminum masking.
(b) Etch cavity with nickel masking. The “grass” is very prominent.

#Reactive Ion Etching

A review of state-of-the-art techniques for anisotropic etching of SiC thin films (Pan & Steckl 1990)123, (Flemish et al. 1996)124, (Wang et al. 1998)125 indicates that RIE with various mixtures of SF6, CHF3, O2 and inert gases successfully etches SiC thin films. Table 2.1 below lists all process runs with their parameters and given etch rates. The first recipe tested was a mixture of CHF3/O2, shown to work well by Pan & Steckl (1990)123.

Etch rate measurement and quality control by  The top bright layer is the metal mask, the light gray layer just below is the SiC film. The silicon substrate is the dark gray layer on the bottom of the image.
Figure 2.6.
Etch rate measurement and quality control by SEM. The top bright layer is the metal mask, the light gray layer just below is the SiC film. The silicon substrate is the dark gray layer on the bottom of the image.
Table 2.1.
RIE parameters fine-tuning for etching heteroepitaxially grown 3C–SiC thin films. The etch rate is mainly dependent on the flow rate of O2 in the chamber. The introduction of argon and power increases have little effect on the etching speed, but considerably improve the wall slope aspect ratio.
RF Power (W) Pressure (mTorr) O2 (sccm) CHF3 (sccm) Ar (sccm) Obtained etch rate (nm/min)
300 20 18 2 0 ~0.0
200 50 45 5 0 17.0
300 150 45 5 0 12.0
200 150 45 5 5 15.0
250 150 45 5 5 15.0
250 100 45 5 5 12.6
150 50 45 5 5 5.4

#3C–SiC suspended wires

Once a satisfactory RIE recipe was settled, a similar process flowchart, detailed in figure 2.7, was established to produce simple SiC resistors. An additional XeF2 isotropic vapor etching step was added after chip dicing to make the wires suspended. Wires of 50, 100, 150, 200, 250 and 500 µm length and 6 µm width were produced this way. A SEM detail of one wire is shown in figure 2.8. Here, the 800 nm-thick epitaxial layer of 3C–SiC was shown to be self-supporting, without depending on an additional mechanical support to achieve wire suspension. Another fabrication test has shown that 1 mm-long wires are also self-supporting. The SiC/Si lattice mismatch works in favor of the wire’s structural integrity, because of the SiC film being strained in tension rather than in compression. As a consequence, the wire is held “taut” by its supports.

3C–SiC heteroetpitaxy on Si Evaporation of Al& lift-off RIE of SiC Al mask removal XeF2 isotropic Si etching –wire release Obtaineddevice Si Al 3C–SiC 200 nm suspendedSiC wire contact pads
Figure 2.7.
Fabrication flowchart for a simple SiC suspended wire.
 detail of one suspended wire.
Figure 2.8.
SEM detail of one suspended wire.

#Remarks on the etching process of SiC

As figure 2.8 shows, the surface quality of the cavity created by XeF2 vapor is quite porous, most likely due to mask redeposition in the cavity floor during the RIE step (figure 2.9 (a)). An attempt to smooth the cavity bottom was made by baking the chips in a tubular oven at 1 300 °C for 15 minutes. As expected, the silicon pores were smoothed out, but silicon nanowires appear to have grown, seeded by the deposited mask particles (figure 2.9 (b)). This is not a limiting issue for this specific process on its own.

(a)  detail of the wire just after the  step with aluminum masking.
(b) The same wire suspended and baked at 1 300 °C for 15 minutes. The white particles have become seeds for nanowire growth.

Figure 2.9.
Side effects of using an aluminum mask for etching SiC.

#2.1.3 Current leakage through the silicon substrate

#Characterization setup

After fabrication, the chips are placed in a Nextron micro-probe station (figure 2.10), which uses needle probe tips to make precise electrical contacts. Current-voltage measurements are performed by a SMU, here a National Instruments PXIe-4142 or a Keithley Model 2450 used interchangeably, plugged into the station’s coaxial ports. The probing station is equipped with a resistive heater buried underneath the test platform, which is regulated for temperature ranging from ambient to 700 °C.

Nextron micro-probe station with heating control, to measure the resistance-temperature characteristics. The measurements are performed with a PXIe-4142 4-channel
Figure 2.10.
Nextron micro-probe station with heating control, to measure the resistance-temperature characteristics. The measurements are performed with a PXIe-4142 4-channel SMU.

Because hot-wire and hot-film sensors rely on the thermoresistive effect, the key indicator of their sensitivity is the TCR. In order to accurately measure it, the electric resistance is probed with the SMU for different substrate temperatures. For metals, where this characteristic is linear, a linear regression gives the slope coefficient, which is divided by the base resistance at room temperature to obtain the TCR. For semiconductors like SiC, the resistance-temperature characteristic is expected to be non-monotonic, and the TCR depends on the temperature and the base resistance R_0 at ambient, with the relation \text{TCR}(T) = \frac{1}{R_0} \frac{\text{d}R}{\text{d}T}.

2026-09-12T13:33:30.693904 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 5 10 15 20 25 Wire resistance (kΩ) linear fit: slope = 517.0 kΩ/cm measurement points 100 200 300 400 500 Wire length (µm) 0.05 0.06 0.07 0.08 M e a s u r e d   r e s i s t i v i t y   (   Ω   c m ) 1 0 − 2 0
Figure 2.11.
Measured resistance and calculated resistivity for SiC suspended wires of various lengths and 6\times0.8 µm section area.

The resistance is measured for each wire length, first at ambient temperature. The results are shown in figure 2.11. The resistance-length characteristic is linear, however there seems to remain a contact resistance of approximately R_\text{c} = 1.9 kΩ. This is likely due to the poor quality of the ohmic contact between the SiC surface and the probe needle. The resistivity of this epitaxial layer of SiC is also much greater than that of metals: a similar geometry made of gold or platinum would be on the order of 100 Ω, whereas here it is on the order of 10 kΩ.

#Resistance drops after 150 °C

The resistance of each wire is measured as a function of temperature; the results for 100, 200, 250 and 500 µm are shown in figure 2.13 (b). While the non-linear aspect of the resistance-temperature characteristic is expected, the measured resistances significantly drop after 150 °C, all reaching near-zero values at 500 °C. This phenomenon is attributed to the silicon substrate acting as a parallel resistance, which greatly decreases as the temperature increases (figure 2.13 (a)). Here, we confirm the well-known issue discussed in the literature review, which prevents the simple measurement of a resistance made of epitaxial layers of SiC on silicon.

#Resistance is heavily light-dependent

As a side effect, the electric resistance also greatly varies relative to light exposure. A simple desk light used on the characterization setup, when switched on and off, makes the resistance jump to ~50 % of its value in the dark (figure 2.12).

2026-09-30T16:24:56.608847 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ lights offµ = 12.723 kΩσ = 4 Ω lights onµ = 6.942 kΩσ = 42 Ω 7 8 11 12 13 Resistance (kΩ) 9 10
Figure 2.12.
Resistance dependence on light for the 200 µm-long SiC wire.

This effect, combined with the fact that some parallel resistance exists via the silicon substrate, makes simple resistors fabricated from 3C–SiC epilayers unusable in thermal sensor applications. The work below seeks to investigate to what extent thermal flow sensors can be fabricated out of silicon carbide.

Figure 2.13.
Current leakage phenomenon observed with SiC/Si wires.

currentin Total resistance decreases when substrate is heated due to leaks through SiC/Si interface. probe needles current through SiC wire leaks through Si substrate SiC currentout Si

(a) Current leakage issue in simple resistors fabricated from a 3C–SiC epilayer.

2026-09-12T13:53:35.281822 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 100 200 300 400 500 Temperature (°C) 0 5 10 15 20 25 Resistance (kΩ) Si layer leaks current wire length (µm) 100 200 250 500

(b) Resistance relative to temperature for the array of SiC resistors. The resistance completely plummets after 150 °C, which is due to current leakages in the silicon.