#2.3 Fabrication of SiC calorimeters

A calorimeter is an array of three parallel wires, placed closely so that they can thermally influence each other. The central wire is used as a heater, and can be used as a single hot-wire sensor, while lateral wires perform passive temperature measurement. Their differential value gives the direction of the flow. Here, for such surface-mounted sensors, it is possible to measure the WSS value and direction. This section details the technological developments conducted to produce such devices, without sacrificing parallel manufacturing capabilities. Indeed, as the literature review indicates, there is, to this date, no reported fabrication process to combine the electric insulation, close placement of the wires, and parallel manufacturing capabilities all at once.

Although the design principle is the same as that of previously presented single wires, bringing three of these in close proximity implies a few process changes. The lateral etching amount induced by the wire release step needs to be brought to a minimum, so the fabrication flowchart established in the previous section cannot be directly adapted to make closely placed wires. Several methods of providing electric insulation are discussed in this section: using a SoI wafer, using a low-doped buried SiC layer and using mechanical lapping and anodic bonding the same way as in the previous section, with a process modification to be able to limit the under-etching amount. It is found that only the latter provides successful insulation, and thermoelectric characterizations are conducted on the produced devices.

#2.3.1 Chip design

A preview of the GDSII file is shown in figure 2.25. The SiC etching pattern is shown in pink/brown. It delimits three insulated zones of SiC, that taper down to the center to form three parallel wires. The metal contact pads are defined by the purple rectangles. Although the lithographic steps were iteratively tested on the Kloé Dilase D650 laser writer, the final design was etched into two 100-mm chromium photomasks, with the help of Jean-Claude Gerbedoen at Institut ONCOLille. This enabled fast, cheap and reproducible lithographic steps, using a Süss MA6/BA6 aligner.

500 µm
Figure 2.25.
Detail of the GDSII design for a single SiC calorimeter chip. In purple, the design for contact pads (positive mask). In pink and brown, the pattern for opening the SiC/Si layers and defining the wires (negative mask).

This design also allows other insulation techniques to be tested, as detailed in the following sections.

#2.3.2 SoI insulation

Using a SoI wafer is the most widely used way to provide electric insulation for critical components, in applications like power and radiofrequency electronics. 3C–SiC layers have reportedly been deposited on SoI substrates by Zappe et al. (2001)100 and Placidi et al. (2010)128, so a similar deposition process to that detailed at the beginning of this chapter was used, in a 4”-capable hot-wall CVD reactor at CRHEA.

#Fabrication

The fabrication process is the same as that presented in figure 2.7. After Ti/Au contact pads evaporation and lift-off, a Cr/Al mask is used to dry-etch the SiC layer. After chip dicing, the final devices are obtained by using four 10-second cycles of 4.5 mTorr of XeF2 pressure. The complete fabrication flowchart is shown in figure 2.26.

Si buriedoxide Si 1 µm 10 µm SoI wafer Poly-SiC deposition Contact pads evaporation RIE of SiC XeF2 wire releaseafter chip dicing 800 nm 250 nm Ti/Au 6 µm 6 µm poly-SiC
Figure 2.26.
Fabrication flowchart of a SiC calorimeter on a SoI base.

#Mechanical integrity of poly-SiC for suspended beams

Unfortunately, the poly-SiC deposition is not mechanically strong enough to self-support into 250 µm-long beams, as figure 2.27 shows. This SiC film seems to have different mechanical properties. Unlike the SiC epilayers grown on bare silicon, this film seems to be in compressive stress, which causes the beams to buckle, eventually touching the bottom of the cavity and making this structure unusable as a sensor.

 detail on the wires of a calorimeter made of poly-SiC deposited on a SoI wafer. The poly-SiC layer is not stiff enough to form self-supported beams.
Figure 2.27.
SEM detail on the wires of a calorimeter made of poly-SiC deposited on a SoI wafer. The poly-SiC layer is not stiff enough to form self-supported beams.

#2.3.3 Highly resistive 3C–SiC buried layer insulation

As the poly-SiC layer used on SoI wafer cannot provide self-supporting beams, a way of producing a SiCoI wafer from epitaxial layers is considered. The underlying hypothesis is that the ~1.12 eV bandgap of silicon implies that around 150 °C, the intrinsic carrier generation starts to dominate, and the electric resistance collapses. To provide insulation, an intrinsic 3C–SiC layer is epitaxially grown first, followed by a more heavily doped one. The 2.2 eV bandgap of SiC would allow for a higher threshold temperature before the carrier generation becomes predominant.

#Heteroepitaxy of a bi-layer of SiC on silicon

The bi-layer is grown in the same reactor and under the same conditions as those detailed at the beginning of this chapter: carbonization of the silicon surface, followed by the 3C–SiC growth step. The only difference lies in the dopant flow. A first layer is grown without any intentional doping, so that it remains highly resistive, then an additional flow of N2 is introduced into the gas phase without interrupting the growth, to produce the n-doped active layer on top. Nitrogen atoms are incorporated on carbon sites of the SiC lattice, where they act as shallow donors. The doping process in this reactor was established by Zielinski et al. (2008)129, who studied the influence of the nitrogen flow rate and growth parameters on dopant incorporation in 3C–SiC films and confirmed its substitutional character. Since the dopant uptake is controlled by the nitrogen flow, both layers can be grown in a single run with a sharp contrast in resistivity.

#Fabrication

The fabrication flowchart (figure 2.28) is, other than the SiC epitaxial growth step, similar to what has been done for the SiC on SoI calorimeter.

Si dopedSiC highly resistive SiC buried layer Si wafer SiC bi-layer heteroepitaxy Contact pads evaporation Ti/Au RIE of the SiC bilayer XeF2 wire release after chip dicing
Figure 2.28.
Fabrication flowchart of a SiC calorimeter using an insulating layer of highly resistive SiC underneath the active SiC layer.

#Insulation capabilities of the buried SiC layer

The resistance-temperature characteristic of the produced device is shown in figure 2.29. The electric resistance is on the order of 500 Ω, which is much lower than what is expected for this geometry of wire, i.e. about 25 kΩ. More importantly, the resistance value collapses after 150 °C, indicating that a parallel resistance, due to the lack of insulation with the substrate, is still present.

2026-09-21T20:46:53.893891 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 0 100 200 300 400 500 600 700 Temperature (°C) 0 100 200 300 400 500 Resistance (Ω)
Figure 2.29.
Resistance-temperature characteristic of the central wire of a 3C–SiC calorimeter insulated with a highly resistive buried layer. The resistance significantly drops after 150 °C, indicating that the SiC/Si interface still leaks current in this configuration.

#2.3.4 Transfer to borosilicate glass

Since the SoI and buried SiC layer insulation methods did not result in electrically insulated, self-supporting SiC wires, the lapping/anodic bonding method is reconsidered. The key idea is to reduce the amount of lateral etch needed to suspend the wires to a bare minimum. The paragraphs below detail how highly anisotropic DRIE of the silicon layer is used, to create thin “walls” of silicon that can be removed using a minimal amount of XeF2 vapor, implying a minimal amount of lateral etching.

#DRIE of 3C–SiC epilayers

As preliminary tests demonstrated, 3C–SiC epilayers are successfully etched by using DRIE, namely a Bosch process, i.e. successive steps of SF6 plasma etch and C4F8 passivation layer depositions, to achieve a vertical etching direction. This creates 6 µm-wide remaining silicon walls supporting the SiC wires, which can be easily removed with a light XeF2 vapor etch. However the SiC etch rate is found to be considerably slower than that of silicon. This requires a 6 µm-thick AZ 15nXT photoresist mask.The lack of O2 in the chamber allows a photoresist mask to be used, which simplifies the overall process.



With a 100 W power, the etch rate of SiC is found to be 2 nm/cycle, compared to ~450 nm/cycle obtained with the same exact recipe on silicon. Overall, after 600 cycles, the totality of the SiC/Si stack is etched.

#Fabrication

A 2-inch 3C–SiC/Si wafer is mechanically lapped on the silicon backside, to a thickness of 50 µm. This thinned wafer is anodically bonded, Si-side, to a 500 µm-thick borosilicate wafer, to produce the base wafer stack. Then, after the Ti/Au contact pads are evaporated, a Bosch process is used to etch through the SiC/Si stack, and, after chip dicing, a final 2-cycle XeF2 vapor etch is used to suspend the wires. Because this process is the converging point of several aspects of the work discussed above, a detailed recapitulating flowchart is shown in figure 2.30. Details of the produced chip are shown in figure 2.32.

LOR 10A / AZ1512optical lithography AZ 15nXToptical lithography AZ 726 MIFdevelopment AZ 326 MIFdevelopment SiC + Si deep etching w/ Bosch process Wafer cleaning + dicing XeF2 wire release on diced chips Perspective view Silicon ⟨100⟩ Si wafer SiCoI wafer preparation Au ohmic contacts patterning Calorimetric structure definition Wire release & final device 1 µm 3C–SiC heteroepitaxy at CRHEA, polished to 800 nm by NovaSiC Backside grinding & polishing 5 nm Ti /250 nm Au evap. Lift-off in SVC-14stripper Anodic bonding to a borosilicate wafer 3C–SiC Borosilicate glass Photoresist Ti/Au
Figure 2.30.
Detailed fabrication flowchart for the 3C–SiC calorimeter made using the lapping and anodic bonding method.

Figure 2.31.
Wafer-level fabrication process and results for 3C–SiC calorimeters using the anodic bonding technique.

<100>Si wafer 3C-SiCepitaxy Backside grinding+ polishing Anodic bonding toa borosilicatewafer Borosilicate Ti/Au padsevaporation DRIE ofSiC + Si XeF2 wirerelease 300 µm 50 µm 800 nm 250 nm 6 µm 6 µm Si 3C-SiC

(a) Fabrication flowchart for the SiC calorimetric WSS sensor, insulated with mechanical thinning of the silicon backside and transfer to a borosilicate substrate.

(b) Resulting 5×5 chip array fabricated on a 2-inch wafer, before saw dicing and wire suspension.

Figure 2.32.
3C–SiC calorimetric sensor, obtained with mechanical lapping and anodic bonding to a borosilicate wafer.

800 nm 50 µm 300 µm 3.4 mm 3C-SiC gold contactpads silicon layer borosilicatesubstrate lateral measurementwires (LW) central heatingwire (CW) 4.9 mm

(a) Schematic representation of the SiC calorimetric sensor chip.

(b)  detail on the array of 250 µm-long, 6 µm-wide parallel wires.

Since this method is the only one tested that properly insulated the SiC wires from the substrate, all characterizations presented in the section below were conducted on calorimeters fabricated this way.

#2.3.5 Characterizations

The tests detailed in the paragraphs below were made on the devices fabricated with the lapping / anodic bonding silicon-side technique, the only one found to be reliable. The three SiC wires are completely electrically insulated and the lateral wires thermally influenced by the central heating wire. As a consequence of the fabrication process and design choices, the lateral wires’ supports are slightly off-centered, which means that the SiC effective length is longer than that of the central wire. This results in a lateral resistance approximately 17 % higher than that of the central wire.

#Influence of the doping levels on the resistance-temperature characteristic

As two batches of calorimeters were produced with different levels of doping, their resistance-temperature behaviors are compared in figures 2.33, 2.34. The resistivity difference is significant, with the lower-doped SiC resistances exceeding the range of the measurement instruments.The Keithley 2450 series has a maximum output voltage of 200 V.



That is why the readable resistance values appear after 150 °C heating, with a 80 MΩ resistance. The higher-doped resistances lie in the 25-30 kΩ range. They show alternating regimes of increasing and decreasing resistance, which can overall be attributed to the semiconducting nature of the material, though the precise underlying phenomenon could not be confirmed.

2026-02-17T14:31:32.143613 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 23 23.5 R e s i s t a n c e   ( k ) Ω 100 200 300 400 500 Temperature (°C) −500 −250 0 250 T C R   ( ) p p m K − 1
Figure 2.33.
Resistance-temperature characteristic and corresponding TCR values for the central wire of a 3C–SiC calorimeter with high levels of doping.
2026-09-19T13:49:22.904022 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 0 25 50 75 R e s i s t a n c e   ( M ) Ω 200 300 400 500 600 700 Temperature (°C) −10 000 −7 500 −5 000 TCR (ppm/K)
Figure 2.34.
Resistance-temperature characteristic and corresponding TCR values for a similar 3C–SiC calorimeter, with a lower level of doping.

The lower-doped resistances present a much higher TCR in absolute value, at about 10 000 ppm/K at 150°C, probably much higher at room temperature, compared to that of the higher-doped resistances. This has some implications for the operation of thermal sensors in CC or CTA conditioners. Most of the hot-film or hot-wire sensors incorporate resistances of about 10-100 Ω, and all currently developed control electronics are designed to operate at these values. A greater electric resistance means that for a given overheat point, i.e. a given power input, the Joule heating voltage value is greater. While the highly-doped SiC resistors at 25 kΩ still offer a workable compromise,a ~30 mW heating power requires a ~30 V actuation voltage



the lower-doped resistors, at around 25 MΩ, would require nearly 900 V to reach the same power level. Although a CTA conditioner suited for the higher doped SiC resistance was designed, as detailed in the next chapter, the lower-doped resistance would require specific component choices and architecture considerations, which is beyond the scope of this work.

For sensor integration into real systems, this means that a trade-off between resistivity, TCR, and wire geometry has to be made. For instance, benefiting from high TCR values brought by low-doped SiC resistances would only be possible for sufficiently short or wide wires, thus reinforcing the thermal conduction effect through the anchor points, as confirmed by the large heater geometry presented by Balakrishnan et al. (2018)115. Considering the current state of the art in conditioning electronics, the fabricated devices best suited for operation in a CTA system seem to be the higher-doped SiC resistance at 25 kΩ, where the TCR is in the ±500 ppm/K range.

#Resistance-power characteristic

As with the simple suspended SiC wires, their behavior under Joule heating is tested. This time, an electrical current is sent through the central heater (CW), whose resistance is acquired by a voltage measurement. The response of lateral wires (LWs) is passively measured, with a 100 µA current, to ensure negligible heating compared to that of the heater. As figure 2.35 shows, the heater presents a convex resistance-power profile similar to that of the simple SiC wire (figure 2.24 (a)), with a different minimum due to the different resistance-temperature characteristic. The lateral wires present a 100 Ω constant difference, due to slight geometry variations during the etching process. However, they equally respond to the heat by presenting a similar convex behavior, offset towards high power values compared to that of the heater. For most of the probed power values, the lateral resistances stay in the negative TCR range.

2026-02-17T14:36:37.777493 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 24 26 28 30 32 C W   r e s i s t a n c e   ( k ) Ω CW 28.0 28.2 28.4 28.6 28.8 L W   r e s i s t a n c e   ( k ) Ω LW1 LW2 0 5 10 15 20 25 30 35 CW heating power (mW) −10 000 −5 000 0 5 000 10 000 P C R   ( ) p p m m W − 1 CW LW1 LW2
Figure 2.35.
Resistances of the central (CW) and lateral wires (LWs), relative to the central wire heating power. The central resistance is measured with its power input current, the lateral ones are measured with a 100 µA current.

Because of the non-constant TCR, the relevant quantity for sensor operation in a CTA is the wire’s resistance variation with respect to Joule heating. The large increasing resistance regime between 20 and 35 mW can be linearized, meaning that a CTA can normally operate in this range. This is why we can consider an equivalent to the TCR called the PCR. Unlike the TCR, the PCR is not an intrinsic property of the material alone but arises from the combined effects of material properties and wire geometry. We therefore propose a PCR curve for each of the three wires relative to the Joule power applied at the central wire. The feedback loop only works for positive PCR values, making the 0 to 5 mW heating range unreachable. Overall, the CTA system achieves optimal sensitivity at the maximum of the heater’s PCR, while the lateral wire measurements are most sensitive when their corresponding PCR reaches peak absolute value.

#2.3.6 Concluding remarks on SiC calorimeters

This chapter detailed the technological developments and results to produce SiC resistors that meet the three objectives drawn from the literature review: electrically insulated, suspended wires produced using only wafer-level steps. It was deduced that, using the materials and deposition techniques available, only mechanical lapping and transferring to a borosilicate substrate succeeds in fabricating such devices. The produced calorimeters were thermoelectrically tested, and the compromise between acceptable resistance values and high TCR was discussed.

The following chapter details tests that were conducted on the SiC devices to assess their behavior in real flows, namely in a static and dynamic WSS calibration setup, and statically in a hot gas generation setup to see potential degradations.