#3.3 Behavior of SiC sensors under temperature

The final part of this thesis explores the sensors’ resistance to temperature, whether brought by Joule heating or by external conditions. The high thermal resilience of SiC presents a double advantage: for probing flows at ambient temperatures, it allows for higher overheat values, resulting in better sensitivities, while also enabling hot flows to be probed. This way, SiC-based probes can have a longer life by reducing the occurrences of fuse-like melting.

#3.3.1 Heating power tests

The SiC resistors’ behavior under cycles of heating/cooling was assessed in the Nextron probe station, using a square current input. Preliminary tests, conducted on the single SiC wire presented at the beginning of chapter 2 (figure 3.10), showed that the sensor reliably handles 13 mW power cycles.

2026-08-26T19:44:04.363655 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 0 20 40 60 80 100 120 Time (s) 0 2 4 6 8 10 12 14 Power (mW)
Figure 3.10.
Thermal stability under cycles of heating for a 18 kΩ single wire, with a 850 µA heating current.
Power test of the calorimeter chip’s heater, producing a visible glow to the naked eye. The current injected is 1.1 mA, which translates to 40 mW of power.
Figure 3.11.
Power test of the calorimeter chip’s heater, producing a visible glow to the naked eye. The current injected is 1.1 mA, which translates to 40 mW of power.

#3.3.2 Hot environment tests

Because the fabricated sensors are SiC/glass composites, the true thermal limits of SiC cannot directly be assessed, as the glass transition temperature of borosilicate happens around 550 °C. The final part of this thesis is a temperature crash test, conducted by baking the sensor chip at 500 °C for several hours and comparing the before/after characterizations. While some tests were conducted at 700 °C, the deforming glass layer induced cracks over the SiC surface, breaking the electrical continuity of the wire, making the sensor chips virtually unusable.

A tubular oven with a quartz tube is used for this experiment (figure 3.12). The sample is placed on an alumina boat, which is slid inside the tube to reach the center of the oven. A 10 °C/minute heating step is applied to bring the oven from ambient to its plateau temperature, which is maintained for two hours. After cooldown, the sample is characterized in resistance-temperature, and inspected with SEM imaging (figure 3.13).

Vacuum pump Gas outlet at ambient pressure Pirani gauge Vacuum pump Tubular oven Gas mixture inlet Quartz tube Aluminasample carrier Sample

(a) Cross-section schematic of the setup.

(b) Photograph of the oven bench.

Figure 3.12.
Oven and gas inlet systems to produce a hot gas atmosphere.

Figure 3.13.
SiC calorimetric chip images and characterizations before and after a 2-hour baking step in helium at 500 °C.

(a)  image of the wire array, before baking.
(b)  detail of the same wire after baking.
2026-10-07T18:40:38.394407 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 100 200 300 400 500 Temperature (°C) 24 25 26 27 28 29 30 R e s i s t a n c e   ( k ) Ω LW1 CW LW2

(c) Resistance-temperature characteristic before baking.

2026-10-07T18:40:38.067704 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 100 200 300 400 500 Temperature (°C) 24 25 26 27 28 29 30 R e s i s t a n c e   ( k ) Ω LW1 CW LW2

(d) Resistance-temperature characteristic after baking. The resistance values remain virtually unchanged.

Figure 3.14.
SiC calorimetric chip images and characterizations before and after a 2-hour baking step in helium at 700 °C, revealing the limitations of borosilicate glass for hot environment applications.

(a)  image of the wire array, before baking.
(b)  detail of the same wire after baking. The glass layer moving underneath caused the SiC film to crack and break electrical continuity between the wires and contacts.
2026-10-07T18:41:09.465447 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 100 200 300 400 500 Temperature (°C) 24 25 26 27 28 29 30 31 R e s i s t a n c e   ( k ) Ω LW1 CW LW2

(c) Resistance-temperature characteristic before baking.

2026-10-07T18:41:09.930075 image/svg+xml Matplotlib v3.10.1, https://matplotlib.org/ 100 200 300 400 500 Temperature (°C) 30.2 30.4 30.6 30.8 31.0 31.2 31.4 R e s i s t a n c e   ( k ) Ω LW1

(d) Resistance-temperature characteristic after baking. Only one lateral wire kept electrical continuity.

#3.3.3 Concluding remarks on high-temperature tests

The heating power and hot environment tests confirm the thermal resilience of the SiC sensing elements. Under Joule heating, the SiC wires withstand repeated power cycles, up to a visible black body glow, without noticeable drift of their resistance. After a two-hour bake at 500 °C, the calorimeter chips show no visible degradation, and their resistance-temperature characteristics remain virtually unchanged (figure 3.13). At 700 °C, however, the borosilicate substrate deforms past its glass transition, cracking the SiC film and breaking the electrical continuity of the wires (figure 3.14). The limiting factor of the current devices is therefore not the SiC itself, but the glass substrate used to insulate it. Replacing borosilicate with a more refractory insulating substrate, such as fused silica, is the next step towards assessing the true thermal limits of SiC thermal sensors.