#1.3 Adapting MEMS thermal anemometers to harsh environments

Flow sensors are of great use both in experimental wind tunnel setups and on onboard systems. They can serve as simple probes to monitor the evolution of the flow state, or be incorporated in more complex control systems, like flow controllers. Flow control is a subdomain of fluid dynamics, which aims at conforming a natural flow to a desired state, using different strategies. It can be implemented through pure geometry, like dimpling a golf ball to reduce its drag force, or placing winglets at the extremities of an airliner’s wings to reduce the lift-induced drag. Reactive flow control is a more advanced strategy, which relies on dynamic actuation based on sensor feedback. Pushed to its limits, reactive flow control has been shown capable of acting as a complete substitute for flight control surfaces, as demonstrated by DARPA’s ongoing experimental CRANE aircraft project.

However, the fragility of MEMS is a limiting factor for their use in real systems. Hence, the most mature technologies deployed in consumer electronics are temperature, acceleration and camera sensors or micromirror arrays, which can be protected from the elements with adequate packaging. In contrast, flow sensors need to be submerged in the environment in order to operate, which poses a major challenge for climbing up the TRL ladder. As a consequence, governmental agencies and aerospace companies were incentivized to work on large scale joint projects to overcome these challenges. In the early 2010s, NATO’s Research and Technology Organization partnered with GRC and major engine manufacturers to produce a framework toward reactive flow control in jet turbine engines (Culley et al. 2009)11. Although it provided experimental results in research prototypes, this research field is still active, as shown by DARPA’s 2023 HOTS project, whose announcement report emphasizes the following catchline (DARPA 2023)1:

“Sensors are everywhere – except in harsh environments too hot for key components.”

Environmental conditions in gas turbine engines presented in NATO’s RTO technical report (Culley et al. 2009)11.
Figure 1.16.
Environmental conditions in gas turbine engines presented in NATO’s RTO technical report (Culley et al. 2009)11.

This project aims at bridging the technological gaps and engineering bottlenecks yet to be overcome in order to fully equip real-world systems subjected to high temperatures. As stated by the announcement report, there is still a trade-off to be made between sensor sensitivity, frequency response and temperature resistance. This is mainly due to two factors:

  1. MEMS technologies for harsh environment applications are not mature enough,
  2. the 125 °C thermal limit imposed by CMOS requires the conditioning electronics to be operated in a separate cold zone, implying that long signal transmission lines induce more electromagnetic noise and frequency bandwidth loss.

The application fields targeted by HOTS are diverse, but the most critical and demanding domain is jet turbine engines. The project sets absolute goals for future deliverables: up to 1-hour operating capability at 800 °C, 90 dB of dynamic range, pressure resolution to 1 Pa and 1 MHz bandwidth. This highlights the fact that currently, there is no reliable technology for anemometry in hot, chemically reactive and abrasive conditions, like the interior of a jet engine. Although technological developments toward these goals started in the 1990s, concurrently with the advances in MEMS anemometry, technological gaps remain to be overcome.

The following paragraphs present the state of the art in MEMS aimed at hot environments. As shown by the literature, silicon carbide is proposed as one of the ideal materials for these applications, and a state of the art on its use in micromachined sensors is established. As a consequence, it is shown that additional challenges remain in the particular field of silicon carbide thermal anemometry.

Figure 1.17.
3C, 4H and 6H polytype structures of SiC. Adapted from (Jiao 2012)76.

B C A 1.89 Å 3.08 Å Si C

(a) Vertical stacking pattern of the 3C cubic (zinc blende) polytype.

B A C B

(b) Stacking pattern of the 4H hexagonal polytype.

B C B A A C

(c) Stacking pattern of the 6H hexagonal polytype.

#1.3.1 SiC as a material for harsh environments

#Material properties

Silicon carbide (SiC) is a compound of covalently bonded silicon and carbon atoms. It is a hard ceramic, discovered by Acheson (1893)77 and originally used as an abrasive suspension for faceting diamond. The crystal structure of SiC presents polytypism, which is a special case of polymorphism where the two-dimensional translations are preserved. All polytypes are composed of the same planar structure, a pavement of silicon tetrahedra with central carbon atoms. Different SiC polytypes are different vertical stacking patterns of this base plane. Although there are more than 250 identified SiC polytypes, the only ones commonly used in the industry are 3C–SiC (\beta-phase, the only known cubic phase), 4H–SiC and 6H–SiC (\alpha-phase), due to the ability to grow them as wafers or thin films (Mehregany et al. 2000)78.

Table 1.1 displays some mechanical, electrical and thermal properties of 3C and 6H–SiC, compared to those of silicon and diamond. SiC generally shows excellent mechanical robustness thanks to its high Young’s modulus, as well as exceptional thermal and chemical stability. At ambient temperature, 3C–SiC is stable, then transforms to 6H–SiC at 1 700 °C, which is stable up to the sublimation point at 2 830 °C. Above 1 200 °C, SiC oxidizes in air in the presence of water vapor, as follows: \text{SiC}~+~2\text{O}_2 \longrightarrow~\text{SiO}_2~+~\text{CO}_2. However, the oxidation rate is very low relative to Si, and it results in the development of a thin, stable SiO2 surface layer.

Table 1.1.
Properties of 3C, 4H and 6H–SiC compared to those of silicon and diamond. Data from Mehregany et al. (1998)79, Camassel et al. (2000)80, La Via et al. (2023)81.
Property 3C–SiC 4H–SiC 6H–SiC Si Diamond
Melting point (°C) 2 830 2 830 2 830 1 415 4 500
Thermal conductivity (W cm-1 K-1) 5 3.7 5 1.5 20
Coefficient of thermal expansion (10–6 K-1) 4.2 4.2 4.2 2.6 1
Young’s modulus (GPa) 448 390–690 448 190 1 035
Hardness (GPa) 35–45 21–30 21–30 12 70–100
Physical stability excellent excellent excellent good good
Bandgap (eV) 2.2 3.2 2.9 1.12 5.5
Electron mobility (cm2/Vs) 1 000 900 600 1 500 2 200
Hole mobility (cm2/Vs) 40 120 40 600 1 600
Breakdown voltage (V) 4 3 4 0.3 10
Dielectric constant 9.72 9.7 9.72 11.9 5.5
Max. available diameter of bulk wafers (inch) 4 8 4 12 2

#SiC coatings for hot and oxidative environments

The exceptional mechanical and thermal properties of the common SiC polytypes make them attractive to use in critical parts of gas turbine engines. Inside a jet engine, turbine blades face the harshest conditions. As their function is to power the drive shaft, they are subjected to the hot exhaust gases expanding from the combustion chamber, as well as extreme centrifugal forces due to rotational speeds. Typical requirements involve 1 700 °C temperatures, Mach 1.25 speed, 10 bar pressure and particle erosion/corrosion (Spitsberg & Steibel 2004)82. Material scientists have engineered high-performance alloys and single-crystal growth processes for the bulk of the turbine blades. However, the conditions being hotter than the phase transition of the alloy, and as debris corrosion would wear out the part, a surface treatment is applied to produce a hard insulating shell. Silicon carbide is often used as the outer coating layer, in the form of woven fibers which are fixed to the surface by a pyrolysis treatment (Zhu 2018)83.

To give another example of SiC usage as a thermal protection outer shell, the wing leading edges of the space shuttles were tiled with a composite material called RCC. It is a stacking of different graphite layers, which are coated with SiC to provide a hard shell as well as thermal oxidation protection.

#SiC as a CMOS alternative for solid-state electronics for high temperatures and radiative environments

The CMOS technology has a working temperature range between –50 and 125 °C inherently due to silicon’s 1.12 eV bandgap. In particular, this means that above 125 °C, the intrinsic carrier concentration generated in the conduction band is too high for a MOSFET to properly insulate in the off state. As a consequence, any conditioning circuit or logic controller has to be relocated if the environments are too hot, which is detrimental to sensor performance, according to DARPA’s HOTS project statement. Silicon carbide benefits from a much wider bandgap, and alongside other wide bandgap III/V compounds like GaN or AlN, is investigated as a CMOS alternative both for high-power and high-temperatures. Additionally, WBG digital CMOS would be much less prone to spontaneous bit flips due to ambient radiation levels, which is particularly significant in space or nuclear applications.

SiC fuel atomizer for gas turbine engines, cast from a micromachined silicon mold by Rajan et al. (1999)84.
Figure 1.18.
SiC fuel atomizer for gas turbine engines, cast from a micromachined silicon mold by Rajan et al. (1999)84.

In the late 1980s, University of North Carolina initiated the developments to use SiC for electronic devices. A MOSFET was successfully made from a 3C–SiC film deposited on 6H–SiC by Palmour et al. (1988)85. In 1986, Palmour and his collaborators founded Cree Inc., to enter the new market created by wide bandgap semiconductors, and patented several SiC MOSFET designs (Palmour 1993)86, (Palmour 1996)87. In parallel, Cree took advantage of SiC’s wide bandgap, which allows light emission in the blue part of the spectrum, to commercialize the first blue LED (Edmond 1990)88. However, the SiC-based blue LED was so inefficient that the true revolution in lighting technology occurred in 1993, with the invention of the GaN LED by Shuji Nakamura. Cree Inc., renamed Wolfspeed in 2021, is currently the market leader in silicon carbide wafers and films, and SiC power components.

#1.3.2 Developments of SiC-based MEMS

#Early SiC MEMS

Mehran Mehregany, who worked at MIT at the time of the first WSS sensor developments, pioneered the technological developments for SiC MEMS aimed at harsh environment applications (Mehregany & Zorman 1999)89. After his thesis work on micromachined silicon mechanisms at MIT, he transposed a commercial accelerometer process to make a WSS balance, at CWRU (Pan et al. 1999)90. In the late 1990s, his team partnered with GRC in an effort to develop a technological field around smart jet engines (Mehregany et al. 2000)91, which means implementing flow control strategies in jet combustion chambers. They successfully used microfabrication techniques to fabricate SiC atomizers for fuel injection, which require very tight tolerances and resistance to abrasion. They tested them at high pressure and erosion rates, and concluded that SiC outperformed silicon and nickel in that particular use case (Rajan et al. 1999)84.

#Silicon carbide electronics and sensors at Glenn Research Center

The CWRU / GRC collaboration enabled the developments of a vertical APCVD reactor for SiC film growth (DeAnna et al. 1998)92 on 4-inch wafers, laying the groundwork for a SiC technological field for both sensors and microelectronics.

Polycrystalline SiC resonators presented by Roy et al. (2002)4, to pave the way toward a SiC  platform.
Figure 1.19.
Polycrystalline SiC resonators presented by Roy et al. (2002)4, to pave the way toward a SiC MEMS platform.

In the early 2000s, Mehregany’s team successfully created a resonant floating mass by depositing APCVD poly-SiC on a SoI wafer, defining an Al etch mask for RIE patterning of the SiC layer (Roy et al. 2002)4. A capacitive transduction scheme was used, similarly to MIT-like WSS balances. The device was characterized in resonant frequency and SiC/Si thermal expansion coefficients, up to 1 000 °C. Ni bond pads and wire-bonding were used to withstand the high temperatures, as its 1 455 °C melting point far exceeds that of gold (1 064 °C). Iterating on this work, Rajgopal et al. (2009)93 fabricated a poly-SiC accelerometer, characterized for a range of 5 000 g and 18 kHz bandwidth.

Packaged 6H–SiC cantilever anemometer reported by Okojie et al. (2004)5.
Figure 1.20.
Packaged 6H–SiC cantilever anemometer reported by Okojie et al. (2004)5.

Over the same period, Robert Okojie’s team at Kulite Semiconductor Products started working on pressure diaphragms for high temperature applications. They reported a 6H–SiC design withstanding 500 °C conditions (Okojie et al. 1998)3. Foreseeing the technological potential, the company patented several SiC-based pressure transducer designs in the 2000s (Kurtz & Ned 2001)94, (Kurtz 2009)95. Robert Okojie joined the silicon carbide research group at GRC in 1999, where the first CVD single-crystal SiC films were deposited on silicon (Nishino et al. 1983)96. He has considerably developed the sensor and electronics technologies since then, particularly aiming at gaining TRL for the SiC devices. In 2006, he patented a complete packaged system comprising a SiC piezoresistive cantilever anemometer (similar working principle to fences or pillars), including the sensing elements, fabrication process and packaging solution (Okojie et al. 2003)97. In the following years, he published reports on SiC device manufacturing methods at GRC, called “CLASSiC” (Okojie 2005)98, which enabled the batch manufacturing of SiC pressure sensors, accelerometers and cantilever anemometers. Simultaneously, he reported the full fabrication, packaging and characterization at 600 °C of the patented anemometer (Okojie et al. 2004)5 (figure 1.20).

6H–SiC  developed by  /  which remained stable 3 000 hours at 500 °C (Neudeck et al. 2009)2.
Figure 1.21.
6H–SiC JFET developed by CWRU / GRC, which remained stable 3 000 hours at 500 °C (Neudeck et al. 2009)2.

Meanwhile, Robert Neudeck’s team at GRC successfully demonstrated the prototype for a 6H–SiC-based JFET, able to withstand thousands of hours in a steady 500 °C environment with unprecedented low rates of failure (Neudeck et al. 2009)2.

As the CLASSiC process could not be applied to \alpha phases of SiC, Okojie presented an uncooled 4H–SiC piezoresistive pressure sensor functioning up to 800 °C, aimed at insertion closer to jet engine combustion chambers to quantitatively monitor the combustion dynamics (Okojie et al. 2015)99.

#SiC technological field in Europe

The increasingly promising opportunities offered by SiC for electronics and MEMS also attracted actors in Europe, where technological activities were created in the early 2000s. Ernst Obermeier’s team at TU Berlin, who did significant work on wall-mounted hot-wire sensors discussed above, pioneered the fabrication of a pressure membrane made of 3C–SiC heteroepitaxially grown on a SoI wafer at Cree Inc. (Zappe et al. 2001)100. They intensively studied the mechanical properties of 3C–SiC films for membrane applications (Pabst et al. 2012)101.

Pirani gauge beam made of a poly-SiC layer by Mo et al. (2021)102.
Figure 1.22.
Pirani gauge beam made of a poly-SiC layer by Mo et al. (2021)102.

The University of Edinburgh started to develop dry etching processes for 4H–SiC (Jiang et al. 2003)103. They collaborated with Mehregany and Zorman at CWRU to produce electrothermally actuated SiC cantilever beams (Jiang et al. 2006)104 from a 3C–SiC layer heteroepitaxially grown on silicon. They iterated on this technology, and very recently reported (as of 2026) a successful picogram mass measurement under steady 400 °C conditions, using an interferometric measurement method (Zhang et al. 2026)105. In parallel, Pasqualina Sarro’s team at TU Delft also collaborated with Mehregany to develop a LPCVD reactor and recipes to deposit thin SiC membranes, originally to leverage SiC’s high elastic modulus to fabricate thin vacuum membranes (Pham et al. 2008)106. This sparked a series of developments around SiC to develop MEMS aimed at harsh environment conditions. In 2010, they reported the fabrication of polycrystalline SiC membranes, with a thickness of 15 nm, for potential use as electron windows (Morana et al. 2010)107. Using this SiC deposition reactor, Sten Vollebregt’s team recently reported the suspension of a 1 mm-long, 6 µm-thick poly-SiC Pirani beam (Mo et al. 2021)102. The stiffness of the SiC layer is not only sufficient to maintain a constant gap along the whole beam length, but also enables steady vacuum pressure measurements at 500 °C.

Another European collaboration between the GES in Montpellier, Aristotle University in Thessaloniki, Greece and Universitat de Barcelona started characterizing 2.5-µm 3C–SiC films heteroepitaxially grown by Cree (Stoemenos et al. 1995)108. In order to produce SiC films in France, the CRHEA started a technological activity in 2000, with the creation and patent of a new hot-wall CVD reactor (Leycuras 2000)6 aimed at producing the conditions for monocrystalline SiC growth on 2-inch silicon wafers. After the developments of an adequate process, they investigated the stress distribution at the SiC/Si interface to reduce the resulting wafer bowing (Zielinski et al. 2007)109. In collaboration with the GREMAN, they developed a novel microfabrication process to produce thin SiC membranes, both with \langle 100\rangle and \langle 111\rangle crystallographic plane orientations (Michaud et al. 2013)110, (Michaud et al. 2016)111, by depositing a LPCVD SiC/Si/SiC heterostructure on a silicon wafer.

The 3C–SiC epilayers grown at CRHEA were used in several technological maturation projects over the 2010s. In the framework of the French NanoSens project, a collaboration between the CRHEA and the LPN focused on fabricating SiC piezoresistive AFM cantilevers. In that case, using SiC allows for a 50 Ω piezoresistance impedance, which simplifies the readout electronics (Boubekri et al. 2014)112. Using a similar design, SiC microcantilevers were tested for hydrogen sensing in radioactive environments within the H2MEMS project (Shanmugam et al. 2022)7. SiC showed itself as a better alternative to palladium or platinum, in terms of aging and reliability. Inside the same project, a partnership between CRHEA and GREMAN investigated the use of these SiC films for CMUT, to extend their use to harsh environments (Portail et al. 2022)113. Since the devices fabricated for this work also iterate on the SiC epitaxial films from the CRHEA, a more complete description of the reactor setup and deposition conditions is presented at the beginning of chapter 2 below.

Figure 1.23.
SiC-based MEMS developed in France using the epitaxial films grown at the CRHEA.

(a) SiC piezoresistive  cantilever developed by Boubekri et al. (2014)112.
(b) SiC cantilever for hydrogen sensing in radioactive environments, developed by Shanmugam et al. (2022)7.
(c)  micrograph of SiC-based  developed by Portail et al. (2022)113 using a novel process technique to fabricate SiC membranes.

#1.3.3 SiC-based thermal anemometers

Despite their efficiency for anemometry in controlled wind tunnel environments, hot wires are extremely fragile and suffer from harsh conditions such as debris, oxidative environments, improper handling, or simply fuse-like melting due to excessive power input. Because they are individually hand-soldered, replacement probes are on the expensive side. At Dantec Dynamics, prices range from €300 for simple single-wire to €6 500 for multi-wire probes with elaborate coating treatments. Glue-on hot films are sold for €1 200 for a five-piece set. More importantly, in harsh environments such as those described above, it is not yet possible to take in situ aerodynamic measurements. Because thermal anemometers cannot be protected by packaging, the materials composing the probe need to be themselves adequate to harsh environments; that is why SiC appears as an interesting substitute for platinum, nickel or tungsten.

#1.3.3.1 Advantages and specificities of SiC for thermal sensing

SiC exhibits much greater resistance to thermal oxidation than metals. Combined with its exceptionally high sublimation point, this allows it to withstand much higher operating temperatures and overheat levels. Consequently, SiC could not only enhance the resilience of thermal anemometers in harsh environments, but also improve their sensitivity by enabling higher overheat setpoints, given that its TCR is sufficiently high.

SiC is a semiconductor, implying that its resistance dependence on temperature depends on many factors, mainly the doping type, dopant species and depth. When temperature increases, the two following competing effects take place.

  1. When temperature increases, the lattice thermal agitation scatters more electrons, thus reducing carrier mobility and increasing resistivity. This is the metallic behavior.
  2. This effect is counteracted by the semiconductor behavior: thermal energy activates carrier generation, which can either be extrinsic with relatively low energy (extrinsic behavior, with dopant depth as characteristic energy), or intrinsic (intrinsic behavior, which depends on the material’s bandgap).

This implies a non-constant TCR, unlike in metals, and a succession of positive and negative TCR regimes depending on the temperature. In that case, the thermoresistive behavior of semiconductors needs to be experimentally measured. In the late 1990s, the incentive to manufacture temperature probes for the ~1 000 °C temperature range led to the fabrication of the first SiC-based devices to replace thermocouples at Saitama University. By using ultrapure polycrystalline CVD, the measured TCR values were remarkably high: –55 000 ppm/K at room temperature (de Vasconcelos et al. 1998)114.

This result highlights the main lever available to tune the thermoresistive behavior of SiC: its dopant concentration. Low-doped or undoped SiC exhibits TCR values well above those of metals in absolute value, which makes it an attractive material for thermistors and, potentially, for thermal anemometry, where the sensitivity scales with the TCR. Low-doped 3C–SiC epilayers have been reported to reach TCR values on the order of 10 000 ppm/K (Balakrishnan et al. 2018)115, compared to about 4 000 ppm/K for nickel. However, as explained above, the TCR of SiC is far from constant: it varies strongly with temperature, and may even change sign, which complicates the operation of such elements as heaters. Moreover, lowering the dopant concentration raises the resistivity of the material, bringing the resistance of a typical hot-wire geometry to the MΩ range, far beyond what conventional CTA controllers can handle. Keeping the resistance acceptable at low doping would require shorter and thicker wires, which moves the design away from the ideal infinitely long hot wire by reducing its length-to-diameter ratio \ell/d, and increases end-conduction losses. The choice of the doping level is therefore a compromise between sensitivity and operability, which is discussed experimentally in chapter 2.

#3C vs. 4H vs. 6H–SiC

Although the mechanical, thermal and chemical properties of 3C, 4H and 6H–SiC are quite similar and offer comparable advantages in their use for harsh environments, their different crystallographic structures imply process-specific constraints. The main technological aspect to consider is the film/substrate compatibility. Poly-SiC can be grown through APCVD, as demonstrated by the floating masses microfabricated at CWRU, and amorphous SiC films have been sputtered on fused quartz at Griffith University (Dinh et al. 2015)116. However, the growth of monocrystalline SiC requires more precise film/substrate compatibility. Currently, the hexagonal 4H and 6H polytypes can only be homoepitaxially grown on their respective substrates. In that case the heterogeneity is brought by the doping type and level, as recent work reports the use of a p-type layer homoepitaxially grown onto an intrinsic 4H SiC substrate for a hot-film-like flow sensor (Dinh et al. 2019)117. In contrast, 3C–SiC crystallizes in a cubic ZnS-type structure, which allows it to be grown heteroepitaxially on silicon. 3C–SiC presents a 4.3596 Å lattice constant, whereas that of silicon’s diamond structure is 5.4310 Å, resulting in a \approx 20 % mismatch. This quite large lattice mismatch results in high film strains, which have been reduced using different techniques detailed below.

Because the chemical heterogeneity of heteroepitaxy gives much more flexibility for MEMS manufacturing than homoepitaxy, the following paragraphs focus on establishing a state of the art of 3C–SiC/Si sensors where the film serves an electrically active function.

In the early days of SiC investigation in France, a collaboration between the CEA-LETI and Université de Montpellier reported a preliminary study on the potential of 3C–SiC heteroepitaxy on silicon for sensing applications (Dezauzier et al. 1995)12. They emphasized that in order to be used for high temperature applications, the 3C–SiC film needed to be electrically insulated from the substrate. As a consequence, producing SiCoI wafers was critical, and the CEA-LETI patent on the Smart-Cut process, originally used to produce SoI wafers (Bruel 1994)118, served to produce such SiC films on large 100 mm wafers (Di Cioccio et al. 1997)119, with a perspective to access the already existing production-scale facilities for silicon. In 1995, the company NovaSiC was created to exploit the intellectual property generated by this SiCoI method. In 2021, they were acquired by Soitec, the company created for Smart-Cut wafers. Currently, they produce SmartSiC wafers and offer post-processing services, like SiC polishing.

Figure 1.24.
Developments conducted by Griffith University to isolate and electrothermally characterize 3C–SiC resistances.

(a)  view of a single-crystalline 3C–SiC resistor transferred to an insulating substrate with  implantation (Dinh et al. 2015)13.
(b)  measurement setup used by Dinh et al. (2015)116 to characterize amorphous SiC (a-SiC) beams.
(c) Wet oxidation technique to produce electrically insulated 3C–SiC resistors. From Phan et al. (2017)120.

#SiC thermal devices developed by Griffith University

A review of the literature suggests that Nam-Trung Nguyen’s team at Griffith University appears to be the only group to have consistently reported developments in SiC-based thermal anemometry. In the late 2000s, Griffith University developed a technological platform on SiC, notably through a CVD process for SiC/Si thin films (Yu et al. 2007)121, (Yu et al. 2007)121. In 2015, Nguyen’s team investigated the thermoresistive properties of a LPCVD amorphous SiC film deposited on fused quartz (Dinh et al. 2015)116 (figure 1.24 (b)). The resistance, measured over a 25 × 25 mm patch by depositing Ni ohmic contacts, presented high values (3 MΩ at ambient temperature), decreasing with the temperature, indicating a large negative TCR between –15 000 and –5 000 ppm/K. The same year, a similar study was conducted with a single-crystalline p-doped 3C–SiC film heteroepitaxially grown on silicon (Dinh et al. 2015)13. The resistance decrease was of similar shape, but in the kΩ-range, with a corresponding negative TCR between –6 000 and –2 500 ppm/K. In order to successfully measure an electrical resistance, they manually transferred each 3C–SiC pattern with FIB implantation, onto a SiO2 substrate (figure 1.24 (a)).

After 2015, Nguyen’s team investigated ways to batch microfabricate insulated SiC resistors, i.e. make SiCoI wafers. Although polycrystalline SiCoI has successfully been made at GRC, the mechanical and thermal properties are far better with monocrystalline SiC. 3C–SiC nanowires were successfully insulated on a SiO2 layer by Phan et al. (2017)120, by dry etching of the SiC epitaxial layer to shape the wire and isotropic oxidation of the silicon substrate, with the oxide layer overflowing underneath the wire (figure 1.24 (c)). In 2018, the same team reported the fabrication and characterization of a thermal calorimetric flow sensor, by anodically bonding a 3C–SiC epitaxy SiC-side to a borosilicate glass wafer (Balakrishnan et al. 2018)115. The resulting sensor showed a high negative TCR between –10 000 and – 20 000 ppm/K. However, since the sensing elements lay on the substrate (figure 1.25), the heating power had to be high, on the order of 50 mW, and the response times were on the order of hundreds of seconds. This is satisfactory for a steady-flow sensor, but since thermal anemometry’s main goal is to catch flow fluctuations, the sensing elements have to be suspended for the response times to be sufficiently low.

3C–SiC calorimetric flow sensor fabrication process insulated with wafer bonding, by Balakrishnan et al. (2018)115.
Figure 1.25.
3C–SiC calorimetric flow sensor fabrication process insulated with wafer bonding, by Balakrishnan et al. (2018)115.

As of 2026, there are no more recent literature reports on the fabrication of such elements, indicating that an engineering bottleneck has yet to be overcome to fully develop a thermal anemometry field around SiC. As discussed, the material could not only bring its exceptional thermal, mechanical and chemical properties to open harsh systems to hot wires, but the semiconductor nature of SiC could also imply a very high TCR, with potential benefits in sensor sensitivity.