#2.2 Electric insulation of 3C–SiC resistors
The fabrication process and characterizations presented in the previous section confirmed the current leakage issue addressed by Dezauzier et al. (1995)12, and the additional developments needed to manufacture SiC thermal MEMS. As the literature review above suggested, some additional work has to be done, and no technological process has yet emerged to massively produce SiC insulated wires at the MEMS level. This section explores two ways of achieving electrical insulation of simple SiC wires, both relying on transferring onto borosilicate glass by anodic bonding, which is an electrically insulating substrate.
#2.2.1 Anodic bonding
#Principle
Anodic bonding is a wafer bonding procedure used to permanently seal sodium-containing types of glass, typically Schott BoroFloat® or Pyrex®, to silicon (figure 2.14). The surfaces of both elements have to be mirror-polished and brought to atomic proximity. Pressure and heat are applied, to bring the glass close to its transition temperature, usually 350 to 400 °C. An electric potential on the order of 1 kV is applied to the silicon side, and a depletion zone is created in the glass layer, close to the interface. A small electric current is induced by the migration of Na+ ions towards the cathode, away from the interface, and O2– ions towards the interface. These ions create Si–O–Si bonds on the interface plane, which permanently seals the two surfaces together.
Working principle of anodic bonding.
The bonding process takes about fifteen minutes, and is monitored by the time evolution of the drift current i_\text{B}. The seal progresses in fronts at the interface, which causes this current to decrease. The process is considered done once the residual current is as low as 10 % of its initial value, which depends on the overall facing surfaces. The bonded stack is then slowly cooled down, and its structural integrity is ensured by the fact that silicon and borosilicates have roughly the same thermal expansion coefficient.
For the work presented below, two anodic bonding platforms were used: a Süss SB8 anodic bonder available at the IEMN cleanroom, and a bespoke setup designed and assembled by our teammate Aurélien Mazzamurro (figure 2.15). It was developed to quickly perform wafer bondings outside of the cleanroom and avoid the crowded reservation schedules.
Custom bonding setup built by Aurélien Mazzamurro, which enabled quick wafer bondings. The two chuck electrodes are visible, and can be heated and pressed together.
#First bonding tests
For the devices presented in the sections below, the anodic bonding step was performed in the Süss SB8 tool. Because the cleanroom staff had already developed efficient bonding recipes, the first successful bonding tests came quickly, with only minor adjustments of the already existing recipes.
The glass wafers are 4-inch 500 µm-thick borosilicate wafers bought from MicroChemicals GmbH. Before any bonding process, the wafers were cleaned with the following protocol:
- cleaning in “Piranha” solution: 3 volumes sulfuric acid for 1 volume hydrogen peroxide;
- cleaning in acetone and isopropyl alcohol;
- low-power O2 plasma on both surfaces to be bonded.
Quarter of a 2-inch wafer bonded to a 500 µm-thick borosilicate wafer. The lighter spots with interference fringes are air bubbles.
The wafers are then anodically bonded as detailed above. The results are shown in figure 2.16. Where there were defects or dust specks, the atomic proximity could not be achieved, resulting in air bubbles. For mechanical support though, this is not a blocking issue.
#2.2.2 Transfer to borosilicate glass SiC-side
As Balakrishnan et al. (2018)115 reported, it is possible to perform an anodic bonding step with a thin SiC interlayer between the two surfaces. Using a similar process, the idea is to transfer the epitaxially grown 3C–SiC sheet to a glass substrate, and be left with a SiC/glass stack, which can be etched as established before. The process for fabricating such a SiC/glass wafer stack is detailed in figure 2.17.
As the produced sample shows, the structural integrity of the SiC layer is greatly degraded by the process (figure 2.18). A potential hypothesis for this phenomenon is the residual tensile stress caused by the epitaxy process itself, which leaves the SiC film stretched on the glass surface. Because the SiC/glass bond quality is not properly ensured, the SiC film delaminates on the glass surface. As the wafer is handled in photoresist spin-coating and metal deposition processes, the surface continues to degrade. To conclude on this method, the transferred sheet was shown to be too unreliable to pursue the device fabrication, and other bonding methods are investigated, as detailed in the paragraphs below.
Fabrication flowchart for producing a SiC/glass stacked wafer with anodic bonding.
|
|
Figure
2.18.
SiC sheet transferred to glass with anodic
bonding, after the removal of the silicon bulk.
#2.2.3 Transfer to borosilicate glass silicon-side
In contrast to what was detailed in the paragraphs above, anodic bonding is mostly used to perform a Si/glass interface bonding. Performing an anodic bonding as-is to produce a SiC/Si/glass stack would be of little advantage in the current configuration, as it would not get rid of the conducting silicon layer. However, reducing the silicon layer thickness to a reasonable amount, on the order of 10 to 100 µm, would enable a reasonable XeF2 isotropic etch to physically separate “islands” in the silicon layer. This would result in a suspended wire, held in place by separated silicon supports, themselves resting on the insulating glass substrate (figure 2.19).
Fabrication flowchart for simple SiC suspended hot wires.
#Mechanical thinning and polishing silicon wafers
For the aforementioned process to work, the silicon bulk should be thinned down as far as possible. The SiC epitaxial layers are grown on 2-inch wafers, which have been cleaved in quarters for these tests. As the wafer thickness decreases, it becomes harder and harder to handle it without completely breaking it, so an approximate target thickness of 50 µm was chosen. The backside thinning was realized on a Logitech PM5 lapping tool.
2-inch wafer thinned down to 50 µm, anodically bonded to a 4-inch, 500 µm-thick borosilicate wafer. The yellow specks are residual NaOH generated from ion migration in the glass, away from the interface.
First, the wafer is glued to an appropriate chuck with wax, then is attached to the tool’s fixture. A cast iron plate rotates, while the fixture presses the wafer to the plate with a given force. A slurry of 3 µm alumina particles is used as grinding material. Quick iterative tests converged to a grinding rate of 10 µm/min with a plate rotational speed of 45 rpm and 1.6 kg force applied to the wafer. Once the desired thickness is achieved, the settings are changed for surface polishing. The plate is switched to a felt one, the fixture pressure is reduced to 800 g and a Logitech SF1 polishing slurry is used. After ten minutes, the grinding scratches disappear, showing a near-mirror finish. The wafer is separated from the chuck by dissolving the wax in a Logitech Ecoclear® solution heated to 80 °C. At this stage, the thinned wafer is 50 µm thick and extremely delicate. After a thorough clean, the polished silicon side is anodically bonded to a borosilicate wafer, to produce a SiC/Si/borosilicate stack (figure 2.20). Because the thinned silicon wafers were too thin to handle the localized force applied by the Süss SB8 tool, resulting in shattering while bonding, all thin wafer stacks were produced in the custom tool.
#Etching of SiC and silicon, and obtained devices
The SiC and silicon are processed the same way as detailed above, except that a much longer XeF2 isotropic etch step is required. The etch rate depends on the surface to be etched. Typically, for a couple of chips, four 10-second cycles with a 4.5 mTorr XeF2 pressure etch 6 µm of silicon. Here, the number of cycles is quadrupled, to achieve the electric separation of the contact pads. This results in large lateral etching and overhanging sheets of SiC, making the structure all the more fragile. The same pattern is used as the one shown in figure 2.7 above, with the same wire lengths. A SEM detail of one wire is shown in figure 2.21.
SEM detail of a suspended and electrically insulated 3C–SiC resistance. The SiC layer flexes noticeably under its own weight, because of the large overhangs created by the lateral etching of the silicon layer underneath.
#2.2.4 Electrothermal characterizations
#Resistance-temperature characteristic
The characterizations presented in the following paragraphs are conducted to check for the proper electric insulation of the SiC suspended wires. The resistance-temperature characteristic of the 50 µm wire is shown in figure 2.22 (a). The wire is placed in the Nextron test chamber and probed with a PXIe-4142 SMU. The heating platform sweeps between ambient and 500 °C, while a constant 100 µA current is injected in the wire: enough to accurately resolve its electric resistance while keeping the Joule heating negligible. There are two distinct regimes. Between ambient and 160 °C, the resistance decreases due to dopant activation. Once the threshold temperature is passed, the metallic effect becomes predominant: the electron scattering due to thermal activation makes the resistance increase again. The corresponding TCR values range from –700 to +750 ppm/K. The resistance increase after 160 °C confirms that the parallel substrate resistance effect has been completely eliminated.
The SiC being n-doped, its resistivity \rho can be expressed relative to the negative carrier concentration n and mobility \mu_e, as follows: \rho = 1/(qn\mu_e) according to Kittel (2018)126. The concentration evolves with T^{-\alpha}\cdot\text{exp}\left(-\frac{E_\text d}{k_\text B T}\right) where E_\text d is the dopant energy and k_\text B the Boltzmann constant, and the mobility evolves with T^{3/2} (Dinh et al. 2017)127. Thus the resistivity depends on temperature as \frac{\rho}{\rho_0} \sim T^{\alpha - \frac{3}{2}} \cdot \text{exp}\frac{E_\text d}{k_\text B T}, which is fitted to the experimental data (figure 2.22 (b)) in the extrinsic regime. This gives an estimated dopant energy E_\text d = 14.14 meV, which is of the correct order of magnitude for this type of semiconductor, compared with the reports of Dinh et al. (2015)13.
Figure
2.22.
Electrothermal characterizations of SiC
resistors produced by mechanical thinning and anodic bonding to
borosilicate glass.
(a) Resistance and TCR evolution relative to the temperature for the 50 µm-long suspended 3C–SiC wire. An extrinsic domain (in yellow) appears, followed by a metal-like domain (in green). |
(b) Corresponding Arrhenius plot of the relative resistivity change vs. temperature. |
Resistance measurements with a desk light and in complete darkness. The desk light lowers the SiC resistance by 5 ppm.
#Resistance-power characteristic
These results show that 3C–SiC resistors can be successfully electrically insulated. Additionally, suspending the wire unlocks its use as a heater for thermal sensing, with reasonable power input. For a second characteristic, the heating platform is kept at ambient temperature, and much higher currents are fed into the wire, ranging from 100 to 1 800 µA. This time, the Joule heating power is non-negligible, and a given temperature profile settles lengthwise along the wire. The temperature change induces a resistivity change, so the resistance evolution against the Joule power is assessed (figure 2.24 (a)).
Because of the non-linear resistance-temperature characteristic, each wire segment is brought to a different temperature, inducing a specific localized Joule power input, so that the average temperature cannot be determined with the total resistance only. This is the main difference between semiconductor and metallic sensing elements when it comes to thermoresistive sensors. Another aspect to consider is that silicon carbide can handle much higher temperatures than metals, without degrading. Figure 2.24 (b) shows such a SiC wire under extreme heating, on the order of 12 mW, with the black body glow visible to the naked eye. After cooldown, the wire shows little to no degradation in its resistance value.
Figure
2.24.
Successful Joule heating of 3C–SiC suspended
wires.
(a) Resistance-power characteristic for the 50 µm-long suspended 3C–SiC wire. |
|
#Light dependency
The light dependency was also assessed by measuring the SiC resistance in the chamber, by comparing the difference between a lid masking the window and a desk lamp illuminating the setup. One hundred measurement points were taken for each case (figure 2.23). The difference is marginal, about 5 ppm, which, assuming a TCR of 1 000 ppm/K, would bias a temperature measurement by 5 millikelvins.
#2.2.5 Concluding remarks on suspended SiC resistors
The suspended insulated 3C–SiC resistor fabrication and characterizations showed the specificities of using silicon carbide instead of metals for thermal sensors.
On the plus side, SiC, when heteroepitaxially grown on silicon, has great mechanical integrity and can hold itself without requiring additional mechanical supports, like a membrane or microbridges. This means that the entirety of the suspended element can be sensitive to the flow, without the need for a “dead” mass. As expected, SiC also shows exceptional resistance to temperature. Although more thorough tests were conducted, as discussed in chapter 3, preliminary Joule-heating attempts made clear that the reachable overheat temperatures could be much higher than those of metals. Finally, process-wise, this workflow keeps the fabrication at wafer level, meaning that parallel manufacturing of insulated suspended SiC wires is possible.
In terms of technical constraints, 3C–SiC epilayers require thorough processing steps to be electrically insulated from the substrate, as the SiC/Si junction has been shown to leak current when heated. By mechanically lapping the silicon backside and anodically bonding it to a borosilicate glass wafer, such insulated and suspended wires could be fabricated. However, the process implies large overhangs in the SiC sheet, that not only weaken the structure, but also prevent the placement of arrays of wires in close proximity. A 50 µm-thick silicon intermediate layer implies that the wire supports have to be separated by at least 100 µm. Since most wall shear stress sensors incorporate multi-wire configurations, as discussed in the literature review, the follow-up of this work is to research a reliable way of producing such architectures with silicon carbide.
The following section details the technological developments that led to a silicon carbide calorimetric sensor, i.e. three parallel wires placed in close proximity. It requires changing the SiC etching step and makes it possible to test other ways of providing electric insulation of the SiC wires.